Magnesium base alloy of composition of 9 wt. % Li, 1,5 wt. % Al composed of alfa and beta (hcp + bcc) phases was cast under argon atmosphere and extruded at 350oC to obtain bars of cross section 12x12 mm intended for Twist Channel Angular Pressing TCAP deformation. TCAP tool consists of helical part in horizontal area of the channel with an angle of lead γ = 30°. The basic aim of use of helix consisted in simulation of back pressure and thus an increase of the extrusion force. Up to 3 TCAP passes were applied at temperatures 160-250C using rotation of samples in the following passes. The extrusion force was measured during the process and it stabilized already in the first stage of pressing and decreased with a number of passes from 190 MPa at the 1st pass down to 120 MPa in the 3rd pass at 160 C. The initial grain size of the hexagonal alfa phase estimated at 20 micrometers. decreased in the following passes at 160C from about 20 micrometers down to 2,3 micrometers after the 1st TCAP pass at 160C and down to 1,5 micrometers after the 3rd pass. The grain size of the bcc phase was initially smaller and of less elongated shape with estimated size at 10 micrometers. Its refinement after TCAP was less pronounced, however it was more difficult to estimate due to different etching of alfa and beta phases during preparation. As extruded alloy possess hardness 61 HV after extrusion, while after TCAP performed at 160C it slightly decreases down to 58 HV after 3rd pass. TEM studies after TCAP passes show presence of dark bands with a high dislocation density in the beta region particularly in the region adjacent to small grains region consisting of alfa and beta phases. The fine grains of the average size below 0.5 micrometers show rather low dislocation density probably due to grain boundary sliding. The crystallographic relationship (001) alfa || (110) beta indicate parallel positioning of slip planes of both phases probably due to partial activation of slip. Electron diffraction indicate increase of grain misorientation with a number of TCAP passes. Stress/strain curves measured at temperature 200oC at progressively increasing crosshead velocities from 10-4 -10-2 s-1 show that the stress stabilizes at different values depending on the tensile deformation rate. One can measure then the flow stress at different strain rates and calculate the strain rate sensitivity coefficient m. Calculated values of strain rate sensitivity coefficient m show that after 1 TCAP pass the m value calculated using flow stress values within strain rates 10-4 – 5 10-2 is equal to 0.31. The sample of the investigated alloy after 3 TCAP passes shows that value of m calculated from the step rate change experiment is equal to 0.47 for the strain rate range 10-5 – 5 10-4. Obtained values are slightly lower than those reported in the literature what may be caused by close to industrial conditions of casting and extruding of alloys, what may influence oxygen content and presence of microcracks forming during extrusion and during TCAP performed at relatively low temperature of 160C. Results obtained show that increasing of number of TCAP passes has a positive effect on superplastic properties not only due to further grain size decrease, but also due to increase of grain misorientation and a decrease of dislocation density in the following passes.
The effect of subsequent annealing on the electrochemical properties of an AZ31 magnesium alloy processed by extrusion and equal channel angular pressing (ECAP) was investigated. The electrochemical properties were evaluated using potentiodynamic tests in corrosion solution of 0.1 M sodium chloride. The electrochemical changes after annealing were correlated with microstructure evolution. The microstructure was analyzed by SEM and EBSD. The dislocation densities were determined by positron annihilation spectroscopy (PAS). The annealing at temperatures ranging from 150 °C to 350 °C resulted in higher polarization resistance in all cases, with a maximum at 250 °C where the value of polarization resistance was ~17% above the value just after ECAP. It seems likely that differences that have been revealed in the microstructure morphology after heat treatment have an impact on the corrosion behavior. Combination of gradual decrease of dislocation density, grain growth and second phase particles dissolution plays the crucial role on corrosion resistance.
A description is given of a possible use of CONFORM SPD (Severe Plastic Deformation) continuous extrusion process by which ultrafine to nanostructured pure titanium can be produced on a continuous basis. The process has been derived from the ECAP technique but, unlike ECAP, it offers continuous production of high-strength wire. CONFORM SPD is also combined with rotary swaging. Rotary swaging provides additional strengthening and imparts final diameter to the wire. Major products include high-strength wire of titanium Grade 2 and Grade 4. Ti Grade 2 with ultrafine to nano-sized grain shows ultimate strength of up to 1050 MPa. Ti Grade 4 reaches ultimate strengths of up to 1250 MPa. These values are twice or three times as high as those found in the unprocessed material. Typical grain size upon processing ranges from 200 to 500 nm. The work describes the CONFORM SPD process and its potential for commercial application and materials properties of high-strength wire of pure titanium.
Equal channel angular pressing (ECAP) method was used for achieving very fine grained structure and increased mechanical properties of AZ31 magnesium alloy. The experiments were focused on the hot extruded alloys. ECAP process was realized at the temperature 250°C and following route Bc. It was found that combination of hot extrusion and ECAP leads to producing of material with significantly fine-grained structure and improves mechanical properties. More experimental results are discussed in this article.
Al-Cu-Mg alloy (Duralumin) has a high strength and used in aerospace industry from the early 19th century. Traditionally, it has been strengthened by dispersed fine precipitates. 3 decades ago, severe plastic deformation (SPD) methods were developed and many researchers were interested in SPD process because it could produce bulk forms of ultrafine or nano-grained materials. High-pressure torsion (HPT) is one of the widely used SPD processes because HPT process can introduce large amount of strain into sample continuously without changing sample dimension. In this research, Al-Cu-Mg-X (X= Zn, Si, Ge) alloys with fixed (Cu/Mg) ratio of 1, were deformed by HPT process and alloys were subjected to aging treatment. The intension is to combine both precipitation hardening and grain refinement using Al-Cu-Mg-X (X= Zn, Si, Ge) alloys and produce material with superior mechanical properties. To estimate mechanical properties, Micro Vickers hardness measurement was conducted. Microstructure observation was carried out using TEM with accelerated voltage of 120kV.
Cu-7%Al alloy subjected to equal channel angular pressing at cryogenic temperature with liquid nitrogen cooling (Croy-ECAP) was treated by annealing. The microstructure and mechanical properties of Cu-7%Al alloy before and after annealing were investigated. It shows that a large number of annealing twins formed in Cu-7%Al alloy subjected to Croy-ECAP. After 300 ℃ and o.5h annealing in Cu-7%Al alloy processed by Croy-ECAP, tensile strength and uniform elongation was increased up to 644 MPa and 7.6% respectively. The enhanced mechanical properties of Cu-7%Al alloy after annealing is attributed to the high density nanosacle twins.